Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultrason® E 2010 G6 UN - PESU-GF30 - BASF

Material Data Center offers the following functions for Ultrason® E 2010 G6 UN:
unit conversion, PDF datasheet print, comparison with other plastics, parameters for material models, CAE Interfaces

Check here, which other Ultrason E datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
中等粘度注塑等级, 具有高硬度和强度, 30 %玻璃纤维增强。
根据ISO 1043: PESU-GF的缩写名称
加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 25 / * cm³/10min ISO 1133
温度 360 / * °C -
载荷 10 / * kg -
模塑收缩率, 平行 0.3 / * % ISO 294-4, 2577
模塑收缩率, 垂直 0.6 / * % ISO 294-4, 2577
ASTM数据
模压收缩率, 平行 0.004 mm/mm ASTM D 955
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 - / 9800 MPa ISO 527
断裂应力 - / 150 MPa ISO 527
断裂伸长率 - / 2.3 % ISO 527
拉伸蠕变模量, 1h * / 9000 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C - / 55 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C - / 60 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C - / 10 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C * / 9.5 kJ/m² ISO 179/1eA
ASTM数据
断裂拉伸强度 140 / - MPa ASTM D 638
断裂伸长率 1.9 / - % ASTM D 638
弯曲模量 9722 / - MPa ASTM D 790
悬臂梁缺口冲击强度, 1/8 in 10 / - J/m ASTM D 256
热性能干 / 已调节单位Test Standard
ISO数据
玻璃化转变温度, 10°C/min 225 / * °C ISO 11357-1/-2
热变形温度, 1.80 MPa 223 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 224 / * °C ISO 75-1/-2
维卡软化温度, B 217 / * °C ISO 306
线性热膨胀系数, 平行 15 / * E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 45 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-0 / * class IEC 60695-11-10
测试用试样的厚度 1.5 / * mm -
Yellow Card 现存 是的 / * - -
厚度为h时的燃烧性 V-0 / * class IEC 60695-11-10
测试用试样的厚度 3.0 / * mm -
Yellow Card 现存 是的 / * - -
燃烧性-氧指数 47.3 / * % ISO 4589-1/-2
ASTM数据
热释放速率, 垂直 40 E-6/K ASTM D 696
DTUL @ 66 psi 215 °C ASTM D 648
DTUL @ 264 psi 212 °C ASTM D 648
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz * / 4.3 - IEC 62631-2-1
相对介电常数., 1MHz * / 4.3 - IEC 62631-2-1
介质损耗因子, 100Hz * / 20 E-4 IEC 62631-2-1
介质损耗因子, 1MHz * / 100 E-4 IEC 62631-2-1
体积电阻率 * / >1E13 Ohm*m IEC 62631-3-1
表面电阻率 * / >1E15 Ohm IEC 62631-3-2
介电强度 * / 37 kV/mm IEC 60243-1
相对漏电起痕指数 * / 125 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 1.6 / * % 类似ISO 62
吸湿性 0.6 / * % 类似ISO 62
密度 1590 / - kg/m³ ISO 1183
密度 1600 kg/m³ ASTM D 792
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 56 / * cm³/g ISO 307, 1157, 1628
加工推荐(注塑)价值单位Test Standard
预干燥-温度 140 °C -
预干燥-时间 4 h -
加工湿度 ≤0.02 % -
注塑熔体温度 350 - 390 °C -
模具温度 150 - 190 °C -
函数
粘度-剪切速度 , Ultrason® E 2010 G6 UN, PESU-GF30, BASF
剪切应力-剪切速度 , Ultrason® E 2010 G6 UN, PESU-GF30, BASF
动态剪切模量-温度 , Ultrason® E 2010 G6 UN (烘干), PESU-GF30, BASF
应力-应变.  , Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
正割模量-应变.  , Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
应力-应变(等时的) 23°C, Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
蠕变模量-时间. 23°C, Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
蠕变曲线 23°C, Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
应力-应变(等时的) 180°C, Ultrason® E 2010 G6 UN (烘干), PESU-GF30, BASF
蠕变模量-时间. 180°C, Ultrason® E 2010 G6 UN (烘干), PESU-GF30, BASF
蠕变曲线 180°C, Ultrason® E 2010 G6 UN (烘干), PESU-GF30, BASF
比容-温度(pvT) , Ultrason® E 2010 G6 UN, PESU-GF30, BASF
拉伸模量-温度 , Ultrason® E 2010 G6 UN (状况), PESU-GF30, BASF
Fatigue strength , Ultrason® E 2010 G6 UN, PESU-GF30, BASF
典型数据
加工方法
注塑, 异型材挤出成型, 片材挤出成型
供货形式
粒料, 自然色
特殊性能
可电镀的
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 150 - 190 °C
injection molding, Mold temperature, recommended: 170 °C
injection molding, Dwell time, thermoplastics: 10 min

Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%

Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)

Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.

It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.